chemical composition
17-4PH, you need to first understand the chemical composition, hardness, density and heat treatment properties of 17-4PH; let senior imports answer the dimensions of the various specifications of the market 7-4PH sheets/strings/bars/pipes/flanges/wires, as well as process flow and even price analysis.
17-4PH high temperature alloy chemical composition
C: 0.04
Si: 0.60
Mn: 0.28
Cr: 16.0Mn: 0.28
Cr: 16.0
Ni: 4.25
Cu: 3.30
Fe: Surplus
Nb: 0.27
17-4PH is martensite precipitation hardened stainless steel. It has high strength, high hardness, good welding performance and corrosion resistance. It has been widely promoted and used in valves, shafts and chemical fiber industries and high-strength components with certain corrosion resistance requirements.
17-4PH characteristics and scope of use:
Precipitated hardened steel type added with copper. Used to manufacture shafts, steam turbines, components.
17-4PH mechanical properties:
Tensile strength σb (MPa): 480℃ aging, ≥1310; 550℃ aging, ≥1060; 580℃ aging, ≥1000; 620℃ aging, ≥930
Conditions Yield strength σ0.2 (MPa): 480℃ aging, ≥1180; 550℃ aging, ≥1000; 580℃ aging, ≥865; 620℃ aging, ≥725
elongation δ5 (%): 480℃ aging, ≥10; 550℃ aging, ≥12; 580℃ aging, ≥13; 620℃ aging, ≥16
cross-section shrinkage rate ψ (%): 480℃ aging, ≥40; 550℃ aging, ≥45; 580℃ aging, ≥45; 620℃ aging, ≥50
hardness: solid solution, ≤363HB and ≤38HRC; 480℃ aging, ≥375HB and ≥40HRC; 550℃ aging, ≥331HB and ≥35HRC; 580℃ aging, ≥302HB and ≥31HRC; 620℃ aging, ≥277HB and ≥28HRC
17-4PH heat treatment specifications and metallographic structure:
heat treatment specifications: 1) Solid solution 1020-1060℃ quick cooling; 2) 480℃ aging, after solid solution treatment, 470-490℃ air-cooled; 3) 550℃ aging, after solid solution treatment, 540-560℃ air-cooled; 4) 580℃ aging, after solid solution treatment, 570-590℃ air-cooled; 5) 620℃ aging, after solid solution treatment, 610-630℃ air-cooled.
17-4PH metallographic structure: the tissue characteristics are precipitation hardening type.